User Tools

Site Tools


projects:nardoragon_suit:head

Differences

This shows you the differences between two versions of the page.

Link to this comparison view

Both sides previous revisionPrevious revision
Next revision
Previous revision
projects:nardoragon_suit:head [2025/08/21 18:56] – [Headshell] equinnprojects:nardoragon_suit:head [2025/09/10 14:21] (current) – [Ears] equinn
Line 68: Line 68:
  
 Print settings for LW-PLA I used (on modified CR-10S with a microswiss direct drive extruder): Print settings for LW-PLA I used (on modified CR-10S with a microswiss direct drive extruder):
-  Extrusion multiplier: 0.52 +  Extrusion multiplier: 0.52 
-  Print temperature: 225 C +  Print temperature: 225 C 
-  Print speed: 50 mmm/s +  Print speed: 50 mmm/s 
-  Retract distance: 0.5 mm +  Retract distance: 0.5 mm 
-  Retract as few times and as little as possible, otherwise the hotend may clog! +  Retract as few times and as little as possible, otherwise the hotend may clog! 
-  Wall loops: 3 +  Wall loops: 3 
-  Infill: 10 % rectilinear +  Infill: 10 % rectilinear 
-  4 top and 4 bottom shells +  4 top and 4 bottom shells 
-  Layer height: 0.2 mm+  Layer height: 0.2 mm
  
  
Line 86: Line 86:
 This resulted in ears that are under 100 grams each, which made a huge difference in comfort. This resulted in ears that are under 100 grams each, which made a huge difference in comfort.
  
 +Printing LW-TPU can be a bit tricky as I learned. It has to be printed very slowly, and it sticks to the build plate extremely strongly, so it has to be removed carefully. 
 +
 +Print settings (on direct drive CR-10S):
 +  * Extrusion multiplier: 0.6
 +  * Retract distance: 3 mm
 +  * Retract speed: 35 mm/s
 +  * Coast to end enabled, distance: 5 mm
 +  * Layer height: 0.2 mm
 +  * Wall loops: 2 (depends on the parts, the bottom part, up to the hole, has 3 perimeters with 0.4 mm nozzle, 2 with 0.6 mm nozzle, but above that only 2 (this stays 2 for the 0.6 mm nozzle as well unfortunately)
 +  * Print temperature: 250 C
 +  * Bed temperature: 45 C
 +  * Part cooling fan : 50 %
 +  * Printing speed: 40 mm/s (with the 0.6 mm nozzle this is too fast, especially for vase mode, had to halve it to 20 mm/s)
 +  * Reduction of print speed for short layer times was enabled (otherwised the ear tips would go melty), was set to 5 sec, with a minimum speed of 5 %